Problem: Agglomeration formation

CauseRemedies
Grain distribution too fine.Contact the powder manufacturer.
Humidity in the powder due to incorrect storage.The powder must be dry and stored at the working temperature.
Sintering in the nozzles caused by a too high Total air pressure.Reduce the Total air pressure to 4 – 5 Nm3/h.
Poor fluidization in the powder container caused by humid compressed air or a clogged fluidizing plate.Check the compressed air for cleanliness, replace the fluidizing